13th International Conference on Fracture June 16–21, 2013, Beijing, China TABLE 3 The Cathodic Current Density Ic,I (mA/cm2) for Inhibited Chemical Cleaning Solution, under Heat Flux of 60 kW/m2. I% is the Inhibitor Efficiency. Interfacial Temperature values are the same as in Table 2. Bulk Temperature (K) 303 313 323 RPM Ic,I I% Ic,I I% Ic,I I% 600 0.65 92 2.3 88 4.2 89.5 1000 0.60 92 1.9 89 3.2 91.8 1400 0.58 91.1 1.7 89.4 2.8 92.4 TABLE 4 The anodic Current Density (mA/cm2) for uninhibited Chemical Cleaning Solution I a,u , Inhibited Solution Ia,I , and the Inhibitor Efficiency I% Under Isothermal Conditions. Temperature (K) 303 313 323 RPM Ia,u Ia,I I% Ia,u Ia,I I% Ia,u Ia,I I% 0 29 1.8 94 46 2.5 97 97 16 83.5 600 7 1.3 81 14 2.3 93.6 40 5.7 86 1000 6.8 1.3 81 15 2.0 86.7 36 4.8 87 1400 7.1 1.3 81.7 15 2.7 82 38 3.5 91
RkJQdWJsaXNoZXIy MjM0NDE=