13th International Conference on Fracture June 16–21, 2013, Beijing, China TABLE 5 The Anodic Current Density (mA/cm2) for Uninhibited Chemical Cleaning Solution under 60 kW/m2 Heat Transfer Rate (The Interfacial Temperatures are Bracketed). Bulk Temperature (K) RPM 303 313 323 600 13 (322.7) 23 (330.5) 63 (339.9) 1000 12 (315.9) 23 (324.3) 58 (333.7) 1400 11 (312.3) 20 (321.6) 48 (331.4) TABLE 6 The Anodic Current Density Ia,I (mA/cm2) and the Inhibitor Efficiency I% for Inhibited Chemical Cleaning Solution, under 60 kW/m2 Heat Transfer Rate. (The Interfacial Temperature Values are the same as in Table 2) Bulk Temperature (K) 303 313 323 RPM Ia,I I% Ia,I I% Ia,I I% 600 1.8 86 4.1 82 12 81 1000 1.6 87 3.7 84 7.8 87 1400 1.4 87 3.3 83 6.0 87